Skip to content
  1. Blog
  2. Standards

Class A vs Class B Lap Splices in CSA A23.3

CSA A23.3 allows the shorter Class A lap only with twice the steel and under half the bars spliced, so a 50 % stagger still needs a 1.3 ld Class B lap.

Calculations referenced in this post

Development length in tension

Required Ld for bars in tension to CSA A23.3-24 Cl. 12.2

Open the calculator →
On this page
Two lap-splice diagrams show overlapping bars and spans labeled Class A 1.0 ld and Class B 1.3 ld

TL;DR

  • A 25M bottom bar in 30 MPa concrete laps 830 mm as Class A and 1080 mm as Class B under CSA A23.3-24.
  • Class A needs at least twice the required steel and less than half the bars spliced within one lap length, so alternate-bar staggering is still Class B.
  • Lap from the full development length, because the excess reinforcement reduction never applies to splice lengths.

You'll learn

  • The two conditions in CSA A23.3-24 Cl. 12.15.2.1 that both have to hold before a Class A lap is allowed
  • Why an alternate-bar 50 % stagger is Class B under CSA A23.3 even though ACI 318 would call it Class A with twice the steel
  • How to size Class A and Class B laps from the full development length, with no credit for excess steel
  • Which splices stay Class B no matter how much steel you add

The lap note “stagger splices 50 %” turns up on a lot of Canadian drawings, and plenty of engineers read it as the ticket to the shorter Class A lap once the bars are oversized. Under CSA A23.3 it isn’t. A Class A lap is 1.0 times the development length, the embedment a bar needs to reach yield, and a Class B lap is 1.3 times. For a 25M bottom bar in 30 MPa concrete, that’s 830 mm one way and 1080 mm the other. CSA A23.3-24 Cl. 12.15.2.1 decides which one you get. The alternate-bar stagger on most drawings lands on Class B every time.

What earns a Class A splice

A lap works by pushing force out of one bar, through the concrete between the two, and into the other, and that push wedges the concrete apart along the bars. One lap on its own handles that fine. But when half the bars in a mat are lapped at the same place, the splitting cracks from neighbouring laps link up into one plane. The extra 30 % of length guards against that. So the code only lets you drop to the full 1.0 times the development length when the laps are lightly stressed and spread out.

Both conditions sit in one sentence. The steel provided at the splice has to be at least twice what analysis needs there, which keeps the bar stress at the lap to about half of yield. And less than one-half of the total steel can be spliced within the required lap length. Both have to hold, so doubled steel with every bar lapped at one place is still Class B, and so is a sparse stagger in a hard-working zone. The table covers members outside yielding regions and Clause 21.

Steel provided over steel requiredShare of bars spliced within one lap lengthClassLap length
2.0 or moreless than one-half (one in three, say)A1.0 times the development length
2.0 or moreexactly one-half (alternate bars)B1.3 times
2.0 or moreall of themB1.3 times
under 2.0anyB1.3 times

That second condition is where the 50 % note goes wrong. “Less than one-half” is strict, which means alternate bars lapped at one location, exactly half, fail it, and you’d need a sparser pattern, such as one in three. ACI 318 writes the same limit as 50 % or less, and that’s likely where the habit comes from.

Left 4 bars, 2 red sections, 1/2 Class B; right 3 bars, 3 red sections, 1/3 Class A

Worked example, a raft bottom mat lapped two ways

Take a raft bottom mat of uncoated 25M bars at 300 mm, in 30 MPa normal-density concrete with 400W steel. The laps sit where the bottom moment is low, between the columns, and the analysis needs 700 \(\text{mm}^2\)/m there against the 1667 \(\text{mm}^2\)/m the mat provides. Bottom bars have far less than 300 mm of fresh concrete under them, so the bar location factor stays at 1.0. The 75 mm of cover and 250 mm clear between lapped pairs put it in the 0.45 case of Table 12.1. You’d expect all that spare steel to shorten the development length too, but Cl. 12.2.5 rules the excess steel factor out for splices, so the lap starts from the full length.

Calculation

Class A or Class B lap for 25M bottom bars in a raft

CSA A23.3-24 12.2.3CSA A23.3-24 12.15.1CSA A23.3-24 12.15.2

Simplified equation, 0.45 case; uncoated bottom bars at 300 mm, 75 mm cover, normal-density concrete, 400W

Inputs
6 input values\(f'_c = 30\) MPa, \(d_b = 25.2\) mm, \(A_{s,prov} = 1667\) mm²/m ...
\(f'_c\)30MPaSpecified concrete strength
\(d_b\)25.2mm25M bar diameter
\(f_{yg}\)400MPaSpecified yield strength of 400W bars
\(A_{s,prov}\)1667mm²/m25M at 300 mm
\(A_{s,req}\)700mm²/mRequired by analysis at the lap location
\(k_\ell k_c k_d k_s k_g\)1.0Bottom bar
Derivation 4 steps
Step 1: Development length, no excess steel factor\(\ell_d = 828.2\ \text{mm}\)
\[\ell_d = 0.45\, k_\ell k_c k_d k_s k_g \frac{f_{yg}}{\sqrt{f'_c}} d_b\]
\[= 0.45(1.0)\frac{400}{\sqrt{30}}(25.2)\]
\(\ell_d = 828.2\ \text{mm}\)A23.3-24 12.2.3
Step 2: Class B lap\(L_B = 1077\ \text{mm}\)
\[L_B = 1.3\,\ell_d\]
\[= 1.3(828.2)\]
\(L_B = 1077\ \text{mm}\)Detail 1080 mmA23.3-24 12.15.1
Step 3: Class A lap\(L_A = 828\ \text{mm}\)
\[L_A = 1.0\,\ell_d \ge 300\ \text{mm}\]
\[= 1.0(828.2)\]
\(L_A = 828\ \text{mm}\)Detail 830 mmA23.3-24 12.15.1
Step 4: Steel provided over steel required at the lap\(A_{s,prov}/A_{s,req} = 2.38\)
\[A_{s,prov}/A_{s,req}\]
\[= 1667/700\]
\(A_{s,prov}/A_{s,req} = 2.38\)
Checks
At least twice the required steelA23.3-24 12.15.2.1PASS
\(A_{s,prov} \ge 2A_{s,req}\) : 1667 ≥ 2(700) = 1400 mm²/m Demand / capacity0.84
Alternate bars lapped togetherA23.3-24 12.15.2.1FAIL
\(n_{spliced}/n < 1/2\) : 1/2 is not less than 1/2, so Class B and 1080 mm laps Demand / capacity1.00
Every third bar lapped togetherA23.3-24 12.15.2.1PASS
\(n_{spliced}/n < 1/2\) : 1/3 < 1/2, so Class A and 830 mm laps Demand / capacity0.67
Watch outThe one-in-three pattern also needs a 50 mm clear offset between adjacent splices (Cl. 12.15.2.2), and this check counts each set as its own location.
Different inputs? Development length in tension runs this check with yours. Run your own bar and concrete →

So even with more than double the steel, the usual stagger still costs you the 1080 mm lap, and only a sparser pattern such as one in three earns 830 mm. That’s 250 mm a lap, close to a quarter of the length. But outside yielding regions Class B lets you lap every bar at one line, a zone 1080 mm long, while three Class A sets and their gaps stretch to about 2.6 m. That counts each set as its own location, which the 50 mm offset implies but the clause doesn’t spell out. So the shorter lap buys a longer splice zone, and Class B is often the simpler detail.

Bar chart compares Class A and B tension lap lengths by bar size against a 300 mm minimum

The gap between the classes grows with bar size, from 90 mm on a 10M to about 350 mm on a 35M. The 300 mm floor only bites on 10M bars, where the computed 297 mm development length rounds up to 300 before the 1.3 goes on.

Where Class A stops being an option

Some splices are Class B however much steel you add. A23.3-24 Cl. 12.15.2.3 makes every splice in a region expected to yield under factored loads Class B, and it still wants less than half spliced with the 50 mm offset. So the plastic hinge zone of a shear wall never gets the short lap. In ductile and moderately ductile walls, Cl. 21.5.4.1 wants at least 1.5 times over the full height. Lap splices aren’t allowed for bars over 35M, apart from two narrow exceptions. Lapped bars that don’t touch must sit within 150 mm or one-fifth of the lap of each other, whichever is less, because a wider gap makes the force travel farther. The strict half rule isn’t new, since A23.3-19 used the same “less than one-half” wording. What 2024 added is the 50 mm clear offset of Cl. 12.15.2.2 and the yielding-region rule.

Grade moves the number too. Switch the raft to 500W and the grade factor of 1.12 stacks on the 25 % higher yield, so the 25M Class B lap grows from 1080 mm to 1501 mm. That matches the 1501 mm a 25M top bar in 500W needs to develop, because the top bar and Class B factors are both 1.3.

Outside Clause 21 members, detail Class B by default and put the 1.3 factor into the lap schedule, because the two Class A conditions rarely line up by accident. Assuming Class A where it doesn’t apply leaves every lap 23 % short. Chase Class A only where the steel is doubled by design and a one-in-three stagger already suits the pour, as in a long mat lapped in a low-moment zone. That stops holding where lap length itself is the problem, in a congested joint or a short pour, and there a mechanical splice, or at a bar end a hooked anchorage, usually beats either class.

Topics
Share LinkedIn X

Disclaimer: This blog post is for informational purposes only and should not be taken as specific engineering advice. Always consult the latest edition of the National Building Code of Canada and relevant CSA standards for your projects.

Quick answers.

Length. Under CSA A23.3-24 Cl. 12.15.1 a Class A tension lap is 1.0 times the development length and a Class B lap is 1.3 times, and neither may be shorter than 300 mm.

No. Cl. 12.15.2.1 requires less than one-half of the total reinforcement spliced within the lap length, plus at least twice the steel required by analysis. Alternate bars lapped together is exactly one-half, so it stays Class B. A one-in-three stagger can qualify.

No. CSA A23.3-24 Cl. 12.2.5 says the As required over As provided factor shall not be applied to splice lengths. Excess steel can only change the splice class, not shorten the development length the lap is based on.

Next up for you.

One short email when a new post goes up. NBCC, CSA and the design checks behind them.